- Pre-clean inspection area with CLEANER SC-30 to remove oil, grease or with wire brush to remove Scale, rust for easier penetration.
- Spray or brush with PENETRANT SC-10 Allow penetration time as per table below.
Area coverage 50Sq mts/ lit. appox. - Wipe Surface Clear, using Cloth Soaked in CLEANER SC-30, Taking care. Penetrant from defect should not be removed
- Shake the Aerosol can vigorously or stir the bulk developer. Spray DEVELOPER SC-20 in thin, uniform film, from a distance of 8 to 12 inches and 6-8 short sections at a time. Allow to dry.
Area coverage 25 Sq mts/ lit. appox. - The vived red colour combined with better capibility action results in sharply defined flaw indication
The
Dye-penetrant method of in spection with flaw test System may be used on materials Such as Aluminium, Magnesium, Barss, Copper, Cast Iron, Steel, Stainless Steel, Ceramic & Certain Plastics.
Minimun Penetration Time For Penetrants, For Parts-Having Temperature of 15C to 35C| Meterial | From | Type of Discontinuity | Penetration Time (Min) | | Aluminium | Casting | Porosity | 5 to 10 | | Cold Shuts | 5 to 10 | | Welds All | Lack of Fution | 5 | | Cracks | 10 | | Magnesium Brass & Bronze | Casting | Porosity | 5 to 10 | | Cold Shuts | 5 to 10 | | Welds Brazed Parts All | Lack of Fution | 10 | | Porosity | 10 | | Cracks & Fatigue Craks | 10 to 20 | | Steel | Casting | Porosity | 10 | | Cold Shuts | 10 | | Eztrution & Forging Welds All | Lack of Fution | 20 | | Porosity | 20 | | Cracks | 20 | | Fatigue Craks | 20 | | Carbide Tip Tools | I | Lack of Fution | 5 | | Porosity | 5 | | Cracks | 10 | | Titanium & High Temp Alloys | All | | 20 | | For Lower Temperature Penetration Time to be Incraesed |
| |
- Each of above product is available in standard 300 gms aerosol cans or 1 & 5 litres carbouys
- Due to continuos development. We reserve the right to modify specification without notice
- Flaw test must be used in a well ventilated space such that Vapours are carried away